Finishing is where a machined part either becomes a product or becomes a return. The variables that matter are not aesthetic: they are dimensional growth, corrosion performance, and how the finish behaves on the edges the machining left behind.
The six finishes we quote most
| Finish | Growth per surface | Salt spray | Best for |
|---|---|---|---|
| Type II anodize | 10–25 µm, half inward | 200–400 h | Consumer aluminium, visible housings |
| Type III hard anodize | 25–50 µm | 500 h+ | Wear surfaces, slides, defence |
| Bead blasting | 0 (removes 5–15 µm) | None | Uniform matte before anodize or paint |
| Powder coating | 60–120 µm | 500–1,000 h | Sheet metal, steel frames, outdoor |
| Zinc plating | 8–15 µm | 96–200 h | Steel fasteners and brackets, cost-driven |
| Electroless nickel | 10–25 µm, uniform | 300–500 h | Complex steel parts, EMI, solderability |
Swipe sideways to see all columns →
What each finish does to your tolerance
Anodize grows roughly half outward and half inward, so a 20 µm coating adds about 10 µm per face — irrelevant on a ±0.1 mm dimension, decisive on a ±0.01 mm bore. Powder coating is the one that catches people out: 80 µm per face on a mating surface is 0.16 mm of interference. Mask threads, bores and mating faces, and put it on the drawing rather than in an email.
Edges are where finishes fail first
Anodizing builds less coating on a sharp edge than on a flat face, and powder coating pulls away from one. A 0.3–0.5 mm edge break before finishing is not cosmetic — it is what stops the coating from chipping in transit. Specify “break all edges 0.3 mm” and you will see fewer shipping claims.
Colour matching
Anodized colour is a chemical process, not a paint code: two batches of the same alloy in the same tank can differ by a Delta-E of 1–2, and 6061 and 7075 will never match exactly. If panels must match across shipments, order them together, or switch to powder coating where RAL numbers are repeatable — and even then, ask for one batch.
Shipping and handling
- Anodized parts scratch each other. Individually bag, or use foam interleaves — bulk in a carton is a guaranteed claim.
- Powder coated parts chip at corners. Corner protectors and a carton with a 20 mm clearance cost less than a replacement air freight.
- Bare machined aluminium stains from fingerprints within days in humid air. If the part ships untreated, wrap it in VCI film.
- Salt spray ratings are test conditions, not a warranty. A 500 h rating on a coastal installation still needs a maintenance interval.
Decide the finish before you decide the tolerance. Retrofitting a powder coat onto a part designed for bare metal is how a 0.05 mm clearance becomes an interference fit.
We hold an approved supplier list for anodizing, powder coating and plating in the Dongguan area, with first-article colour and thickness checks on every batch. Send the drawing and tell us the environment the part lives in — indoor, coastal, chemical, or handled daily — and the finish follows from that.